how-to-weld-aluminum-to-aluminum
Home Blog How to Weld Aluminum to Aluminum: Prep, Process and Fixes
Repair & Troubleshooting Nov 9,2026

How to Weld Aluminum to Aluminum: Prep, Process and Fixes

Once a trailer repair has been assessed and approved, the work order should carry the job from material identification and fit-up through documented inspection. Use this workflow to prepare an approved aluminum weld, set up the equipment, and verify the finished repair before releasing the trailer. Start with the guide to deciding whether an aluminum trailer part can be welded if the repair route is still open.

Table of Contents

Match the Filler Wire to Your Aluminum Alloy

Record the alloy and temper of both parts from material markings, certification or verified supplier records. If the material is unknown, pause the repair and obtain positive identification or the manufacturer’s disposition. A trial weld on scrap may help evaluate a known setup, but it cannot identify an unknown alloy or approve work on a load-bearing part.

Guessing from the trailer brand or using the wire that's loaded is how shops create cracks they can't see. Different series behave differently in the puddle, and the wrong chemistry follows the joint into service.

What the Common Pairings Take

Use the Lincoln Electric trailer welding guide to understand why filler varies by base-alloy pairing. The examples below are inputs for selecting and documenting the approved procedure. Confirm both alloys, joint strength, service temperature and exposure before selecting the wire.

Base alloy Filler wire Notes
6XXX series, such as 6061 ER4043 An example for compatible 6xxx joints. Check both alloys, temper and service requirements.
5052 ER4043, ER5554 or ER5356 Options Lincoln lists for 5052 joined to itself. Confirm the actual pairing.
5083 joined to itself ER5183 or ER5556 for higher-strength joints Verify required joint strength and service conditions. Other 5xxx pairings may call for different filler.
5154 or 5454 joined to itself ER5554 An example Lincoln lists for these same-alloy pairings.
7075 Stop and obtain manufacturer or engineering guidance High risk of hot cracking in conventional fusion welding. A trial coupon alone does not establish a field repair.

For 5154 or 5454 joined to themselves, 5554 is identified as the appropriate filler. For 5052, you have options, but options aren't permission to pick at random. Consider the load, corrosion exposure, and whether the part flexes.

7075 requires a separate decision. Lincoln cautions against conventional arc welding because of cracking risk. A laboratory study of AA7075 with nano-treated filler used a specialized process. For a trailer part, refer to the manufacturer or responsible engineer for the permitted repair or replacement.

What a Wrong Filler Changes

An incorrect filler can affect strength, ductility, corrosion behavior, and cracking resistance. On a fleet trailer, that shows up as a joint that looks fine in the bay, then cracks beside the bead after weeks of road shock, or corrodes faster around a Walking Floor slat or floor component exposed to wet waste and road film.

Practical rule: Match the filler to the base metal, not to the trailer brand or the wire already on the spool.

Write the alloy and filler on the work order. If the next technician can't tell what was used, you don't have a repeatable repair, you've got a mystery joint.

How to Prep and Fixture the Joint

Prep isn't housekeeping. On aluminum, it's half the weld. Road film, hydraulic residue, paint, and oxide all end up in the puddle if you don't remove them, and the joint pays for it under repeated loading.

A three-step infographic showing how to prep and fixture aluminum plates before performing a weld.

Preparation overview. Use the approved joint opening, fixture, cleaning sequence and hot-work controls for the actual repair.

Work through this sequence in order:

  1. Identify and mark: Confirm the alloy and mark the joint area so no one grinds it with a steel tool. A misidentified part gets the wrong filler and the wrong heat plan.

  2. Degrease first: Remove contamination using the approved cleaner and preparation method. Follow the cleaner’s safety data sheet. Keep it away from ignition sources and remove residue and vapors before hot work. Hydrocarbon contamination can contribute to porosity.

  3. Brush the oxide: Use a stainless-steel brush dedicated only to aluminum. A brush that touched steel leaves ferrous contamination that promotes defects and corrosion. Brush shortly before welding, not the day before.

  4. Recheck before welding: Inspect both mating faces for moisture, dust or residue. Repeat approved cleaning away from ignition sources if needed, then verify that the joint is dry and vapors have cleared.

  5. Fit to the joint detail: Verify edge preparation, bevel, alignment and root opening against the approved procedure.

  6. Clamp and tack: Hold alignment and the specified opening. Follow the approved tack and welding sequence to manage restraint and movement.

  7. Protect the filler: Keep wire and rod dry, capped or bagged, and handle them with clean gloves that haven't touched steel, grease, or grinding dust.

The Go or No-Go Check

Before you strike an arc, verify the joint is clean and dry, the required fit-up is recorded, and solvent vapors and residue have cleared. Confirm the hot-work area is ready before energizing the equipment.

If you see any of those, stop and clean again. Welding over contamination to save ten minutes is how you create porosity and lack of fusion that you then have to grind out and redo.

Clean metal isn't optional on aluminum. It's the difference between fusion and a bead sitting on top of dirt.

Machine Settings for TIG and MIG Aluminum Welds

Start with the machine and torch documentation and the approved welding procedure for this alloy pair, temper, thickness, joint and position. A representative coupon can help demonstrate a procedure when required. Release of the actual part still depends on the manufacturer’s guidance and the repair’s acceptance criteria.

The Lincoln Electric trailer guide gives 35 SCFH for GMAW and 25 SCFH for GTAW in its setup guidance. Miller’s truck repair guide gives 15–20 CFH for flat-position aluminum TIG and different values in other conditions. Treat these as examples from their respective guidance. Set gas and preheat for the actual equipment and approved procedure.

Setting MIG (GMAW) TIG (GTAW)
Shielding gas Approved inert gas and flow for the machine, nozzle and joint Approved inert gas and flow for the torch, cup and position
Polarity or transfer Transfer mode specified by the procedure and supported by the machine Commonly AC. Set starting mode and balance per the equipment and procedure.
Filler or wire Approved filler diameter with a compatible aluminum feed system Approved filler for the actual alloy pair and joint
Wire-feed speed Set for the wire, transfer mode and approved procedure Not used
Amperage Use the approved range and verify on a representative coupon when required. Use the approved range and verify on a representative coupon when required.
Torch technique Use the travel angle, arc length and speed specified for the joint Follow the specified torch and filler technique
Preheat Use only if specified. Record the required range and measured temperature. Use only if specified. Record the required range and measured temperature.

Reading the Table Correctly

For MIG, match the shielding gas and flow to the nozzle and approved process. Confirm a spool gun, push-pull setup or other compatible feed system as specified for the machine and wire. Excess flow can disturb shielding.

For aluminum TIG, AC is common. Set the start mode, polarity balance and gas flow from the machine guidance and the approved procedure. Surface preparation remains part of the process.

Record the settings used on the actual job. If qualification is required, keep the coupon material, settings and results with the procedure record.

Record the Coupon

Log these items every time you qualify a setup:

  • Amperage and travel speed: The pair that gave fusion without burn-through.

  • Gas flow and filler: Exact flow setting and filler designation.

  • Interpass temperature: Measured, not estimated by hand.

  • Inspection result: Visual findings and any bend, penetrant, or other test outcome.

Keep the coupon record with the qualified procedure and separately document inspection of the actual repair before release.

Safety Setup Before the Arc

Set up for safety before the arc, not after someone's already been flashed or a solvent can catches heat. Run this checklist on every aluminum job, even a small bracket.

  1. Eye and skin protection: Wear a welding helmet with the correct shade, flame-resistant clothing, and welding gloves. Put screens or curtains up so technicians in the next bay aren't catching arc flash while they work on brakes or hydraulics.

  2. Ventilation: Assess the work area, coatings and exposure before welding. Set up suitable ventilation or local exhaust and the required protection. For restricted or confined spaces, apply the site’s applicable entry, atmospheric and ventilation controls before work. See OSHA’s welding and hot-work requirements.

  3. Gas cylinder security: Chain or strap the shielding-gas cylinder upright, and check the regulator, hoses, and connections for leaks before you open the valve fully. A leaking hose also ruins gas coverage at the weld.

  4. Solvent separation: Follow the cleaning product’s safety data sheet and OSHA’s precautions for cleaning compounds. Keep solvents away from hot work and verify that residues and vapors are clear, including in seams and enclosed areas.

  5. Electrical check: Inspect the machine ground, leads, and torch for cuts, loose connections, and damaged insulation. A poor ground gives you an unstable arc and a shock risk at the same time.

  6. Fire control: Check both sides of the joint, clear or shield combustibles and arrange extinguishing equipment and a fire watch where required. If the hazards cannot be controlled, stop the hot work.

  7. Hot metal discipline: Mark hot parts and let them cool before handling. Hot aluminum looks cool long after the arc stops, so it burns hands that would never grab glowing steel.

The Trailer-Specific Risks

Check what's inside and under the unit before you weld. Walking Floor trailers and waste haulers can carry residue, hydraulic oil, and trapped debris near floors and sidewalls. Clean and inspect the back side of the joint, not just the face you're welding.

Shop reminder: If you can't see the back side, you don't know what's going to smoke, burn, or contaminate the weld.

Brief anyone working nearby. A helper holding a panel needs the same eye protection and a clear signal for arc start, not a shout after you've already struck it.

Run the Weld, Fix Defects and Finish

Run aluminum in controlled segments and watch fusion, not just bead shape. Aluminum conducts heat away fast, then the whole area gets hot at once, so your technique has to manage both ends of that problem.

An infographic showing TIG welding steps, MIG welding adjustments, and a table of common welding defects.

Common checks to discuss during setup. Use the approved weld and rework procedure for the joint and verify the required acceptance criteria.

TIG Run, Step by Step

  1. Start clean: Use the specified start mode and a clean, properly prepared tungsten for the approved TIG procedure.

  2. Follow the weld sequence: Use the segment length and sequence specified for the joint and monitor heat accumulation.

  3. Feed at the leading edge: Add filler at the front of the puddle without touching the tungsten.

  4. Control the arc at the sidewalls: Follow the specified torch motion, travel speed and heat input for the joint. Verify fusion by the required examination.

  5. Fill the crater: Taper current at termination instead of snapping the arc off.

  6. Shield while hot: Keep argon flowing over the weld until it solidifies.

  7. Cool between passes: Let the joint cool and check interpass temperature before the next pass.

Use the approved procedure to define settings, coupon requirements and inspection. Record the result of each required examination and the acceptance criteria used to release the part.

For MIG, follow the approved technique, gas and heat-input range. If the joint shows lack of fusion or burn-through, stop and assess the cause before rework.

Defects, Causes and Fixes

Symptom Likely cause Fix
Porosity (small holes or pores) Hydrogen from moisture, hydrocarbons, or contaminated filler or gloves Degrease, brush with a dedicated stainless brush, use dry filler, check gas coverage
Lack of fusion Oxide, contamination, poor fit-up or unsuitable heat input or technique Identify the cause and repair the defective area using the approved procedure.
Edge melting or burn-through Amperage set too high Check the fit-up and settings against the procedure before approved rework.
Crater cracks Abrupt arc termination Taper current at the end of each segment to fill the crater
Distortion Heat building in one area Check the fixture and approved weld sequence.
Weak joint under load Softened heat-affected zone, wrong filler, or excess preheat Hold the part for review of the alloy, procedure and required examination.

An AWS Welding Journal study of 2014 and 2219 GTAW welds identified moisture or hydrogen as contributors to porosity in the tested welds. Heat can also soften the heat-affected zone in some heat-treated aluminum alloys. Evaluate the actual alloy, temper and joint using the approved inspection plan.

Inspect and Finish

Inspect accessible surfaces for cracks, undercut, burn-through and porosity. Visual inspection and dye penetrant, where specified, address surface indications. Use the examination specified for internal discontinuities and verify the applicable acceptance criteria before return to service.

Clean spatter and residue with the dedicated stainless brush, remove sharp edges that can start fatigue cracks, and protect the repair from moisture until it returns to service. Document what you found, even when the answer is no defects.

Decide Whether to Weld, Test or Replace the Part

Determine whether the damaged part carries load and check the manufacturer’s instructions for the specific trailer. For covered commercial motor vehicles, 49 CFR § 393.201(d) requires welded frame repairs to follow the vehicle manufacturer’s recommendations. Keep a safety-critical part out of service pending the approved repair, replacement or disposition.

Start by recording the damage in place:

Repair, test or replace a trailer part. Confirm the alloy, load path and manufacturer guidance. Use the approved procedure and resolve unknowns before release.

Run the Decision Criteria

  • Alloy and temper: If either is unknown or difficult to identify, testing or replacement may be safer than choosing filler by guesswork.

  • Thickness: Thin sheet is prone to distortion; thick sections require evidence that the joint has adequate penetration.

  • Joint type: Check the joint geometry, direction of loading, fatigue exposure and approved design.

  • Cyclic loading: Repeated flex in rails, floor supports, and Walking Floor components can challenge the heat-affected zone.

  • Distortion tolerance: A warped floor or sidewall can create operating problems beyond the original crack.

  • Structural role: Check the load path, permitted repair and release criteria with the manufacturer or responsible engineer. Replace the part when the applicable instructions require it.

Springer's friction-stir welding subject collection explains that friction-stir welding avoids melting and can produce high-quality joints. The process is not available for every repair, but it highlights the trade-off: another fusion pass adds heat, while mechanical reinforcement or replacement may better suit a sensitive part.

Repair only where the approved procedure covers the actual part. Resolve uncertainty through the specified evaluation or testing, and replace the component when the manufacturer or approved engineering disposition calls for replacement.

Record the joint location, alloy and temper, thickness, load path and the manufacturer’s disposition. Attach the procedure and inspection record to the work order before releasing the trailer.

Brothers Truck Trailer Repair and Welding Corp. offers aluminum welding for trucks and trailers, including repair of aluminum trailer bodies and components. Its welders have specialized aluminum expertise, and the work is designed for structural integrity and corrosion resistance. For a cracked body, floor, rail, or custom component, contact Brothers Truck Trailer Repair and Welding Corp. about its aluminum welding and custom fabrication services.